Steel comparison · maker data checked 2026-10-21Blue #1 vs Blue #2
Aogami #1 has more carbon and more tungsten than Aogami #2 — 1.25–1.35% carbon and 1.50–2.00% tungsten, against 1.05–1.15% and 1.00–1.50%. Everything else Proterial publishes is the same: the same heat-treatment temperatures, the same delivery hardness (229 HBW or under) and the same hardening hardness (60 HRC or over). Neither is stainless.
Side by side
| Aogami #1 | Aogami #2 | |
|---|---|---|
| Maker | Proterial | Proterial |
| Type | Carbon | Carbon |
| Stainless | No | No |
| C % | 1.25–1.35 | 1.05–1.15 |
| Si % | 0.10–0.20 | 0.10–0.20 |
| Mn % | 0.20–0.30 | 0.20–0.30 |
| Cr % | 0.30–0.50 | 0.20–0.50 |
| W % | 1.50–2.00 | 1.00–1.50 |
| P % | ≤0.025 | ≤0.025 |
| S % | ≤0.004 | ≤0.004 |
| Maker HRC | ≥60 | ≥60 |
| CATRA mm | not tested | not tested |
Mass %, steelmakers’ published typical or representative values. † retailer values or claims (the maker does not publish them). Maker HRC is the hardening hardness the steelmaker publishes, not the hardness of a finished knife. CATRA: Knife Steel Nerds edge-retention test, total card cut. PM = powder metallurgy.
Grind them: the spark test
Steel shops tell steels apart by touching them to a grinding wheel. More carbon makes bushier, forking sparks; tungsten-rich steels throw fainter, redder streaks; high-chromium stainless steels give fewer, more orange sparks that fork only near the ends. Press harder and the sparks get longer — but the pattern stays.
Illustration, not a measurement. The direction of each effect follows published spark-test descriptions (spark testing). The faint red streaks are described for high-speed steels with far more tungsten; for the 1–2.5% in Blue steels we scale the effect down, which is our assumption. Carbon, tungsten and chromium are the steelmakers’ figures from the table above. Spark testing sorts steels; it cannot identify one exactly.
Where the alloy ranges overlap
What the data says
- Both are Proterial (formerly Hitachi Metals) Yasugi Specialty Steels, described by the maker in the same words: alloy steel with tungsten and chromium added to improve heat-treatment properties and wear resistance.
- The only differences in the published composition are carbon (1.25–1.35% vs 1.05–1.15%), tungsten (1.50–2.00% vs 1.00–1.50%) and the lower end of the chromium range (0.30–0.50% vs 0.20–0.50%). Silicon, manganese, phosphorus and sulphur limits are identical.
- Proterial gives both grades the same standard heat treatment: annealing at 750–780 °C, quenching from 780–830 °C in water (or oil), tempering at 160–230 °C. Both are delivered at 229 HBW or under and rated 60 HRC or over after hardening.
- Proterial’s own application lists differ slightly: Aogami #1 for “highest quality” planes, tipped tools, razors and kitchen knives; Aogami #2 for “high quality” planes, tipped tools, kitchen knives and sickles.
- Knife Steel Nerds explains that in these tungsten steels wear resistance is controlled mainly by the tungsten-carbide fraction, while extra carbon mostly adds cementite, which lowers toughness with little gain in wear resistance. On that reasoning, #1 should resist wear more and #2 should be somewhat tougher — but no published test measures the two side by side.
- Knife Steel Nerds also notes that ease of sharpening is the inverse of wear resistance, which would make #2 a little easier on the stones; we found no controlled test comparing the two.
- Neither grade has a published CATRA edge-retention result. The only Blue steel in Knife Steel Nerds’ CATRA set is Aogami Super.
Why the knifemaker matters more than the number
Proterial publishes a hardening hardness of 60 HRC or over for both grades, but the finished hardness of a knife — and therefore how it behaves on the board — is set by the smith’s forging, quench and temper. Two Aogami #2 knives from different makers can differ more than an Aogami #1 and an Aogami #2 from the same maker.
In Sakai, forging and hardening, sharpening and handle fitting are traditionally separate trades (see our history of Sakai knives). When a shop lists “Aogami #1”, it is telling you the steel the smith started with, not the hardness he finished at. If the shop publishes the HRC, that is the number to compare.
Both are usually clad
Kitchen knives in Aogami #1 and #2 are most often made with a core of the paper steel forged between softer iron or stainless cladding (kasumi, san-mai or warikomi construction). The cladding decides whether the sides of the blade rust; the core decides the edge. A “stainless-clad Aogami #2” knife still needs its edge dried after use.
Which should you choose?
| If… | Look at |
|---|---|
| You want the most wear resistance of the two, as the maker’s alloying implies | Aogami #1 |
| You want a little more forgiveness against chipping and easier sharpening, by the reasoning above | Aogami #2 |
| You want more carbon and tungsten again, plus vanadium | Aogami Super |
| You do not want a knife that rusts | Neither — look at Ginsan, VG-10 or SG2 |
The steel is only part of a knife: the knifemaker’s heat treatment, the blade geometry and the edge angle matter as much. See all steels in the Japanese knife steel chart, compare Japanese knife shapes, and if you are ordering from Japan, check the import duty calculator and buying guide first.
Frequently asked questions
- Is Blue #1 better than Blue #2?
- Not simply. Aogami #1 has more carbon (1.25–1.35% vs 1.05–1.15%) and more tungsten (1.50–2.00% vs 1.00–1.50%), which points to more wear resistance; Aogami #2’s lower carbon points to a little more toughness. Proterial rates both at 60 HRC or over and lists both for kitchen knives.
- Is Aogami #1 harder than Aogami #2?
- Proterial publishes the same hardening hardness for both — 60 HRC or over — and the same heat-treatment ranges. A finished knife’s hardness is set by the knifemaker.
- Does Blue #2 steel rust?
- Yes. Aogami #2 has only 0.20–0.50% chromium, far below the roughly 10.5% that makes a steel stainless. Dry it after use and expect a patina.
- What is the difference between Blue #2 and White #2?
- They have the same carbon (1.05–1.15%). Blue #2 adds 1.00–1.50% tungsten and 0.20–0.50% chromium, which the maker says improves heat-treatment properties and wear resistance. See our Blue vs White steel comparison.
More comparisons
- Blue vs White steel
- Aogami Super vs SG2
- VG-10 vs SG2
- White #1 vs White #2
- VG-10 vs AUS-10
- Aogami Super vs Blue #2
- Ginsan vs VG-10
- HAP40 vs SG2
- SLD vs VG-10
Sources
- Proterial grade page
- Proterial grade page
- Knife Steel Nerds: is Blue Super actually super? (tungsten carbides, carbon and toughness) (secondary)
- Spark testing: how carbon, tungsten and chromium change grinding sparks (Wikipedia, with its references) (secondary)
Checked 2026-10-21. Found a better source or an error? Tell us.