Steel comparison · maker data checked 2026-10-21White #1 vs White #2
The only published difference is carbon: Shirogami #1 has 1.25–1.35% and Shirogami #2 has 1.05–1.15%. Proterial describes #1 as “highest hardness” and #2 as “high hardness”, with the same hardening hardness of 60 HRC or over and the same heat treatment. Both are plain carbon steels with no chromium and rust if left wet.
Side by side
| Shirogami #1 | Shirogami #2 | |
|---|---|---|
| Maker | Proterial | Proterial |
| Type | Carbon | Carbon |
| Stainless | No | No |
| C % | 1.25–1.35 | 1.05–1.15 |
| Si % | 0.10–0.20 | 0.10–0.20 |
| Mn % | 0.20–0.30 | 0.20–0.30 |
| P % | ≤0.025 | ≤0.025 |
| S % | ≤0.004 | ≤0.004 |
| Maker HRC | ≥60 | ≥60 |
| CATRA mm | not tested | not tested |
Mass %, steelmakers’ published typical or representative values. † retailer values or claims (the maker does not publish them). Maker HRC is the hardening hardness the steelmaker publishes, not the hardness of a finished knife. CATRA: Knife Steel Nerds edge-retention test, total card cut. PM = powder metallurgy.
Grind them: the spark test
Steel shops tell steels apart by touching them to a grinding wheel. More carbon makes bushier, forking sparks; tungsten-rich steels throw fainter, redder streaks; high-chromium stainless steels give fewer, more orange sparks that fork only near the ends. Press harder and the sparks get longer — but the pattern stays.
Illustration, not a measurement. The direction of each effect follows published spark-test descriptions (spark testing). The faint red streaks are described for high-speed steels with far more tungsten; for the 1–2.5% in Blue steels we scale the effect down, which is our assumption. Carbon, tungsten and chromium are the steelmakers’ figures from the table above. Spark testing sorts steels; it cannot identify one exactly.
Where the alloy ranges overlap
What the data says
- Both are Proterial Yasugi Specialty Steels, described by the maker as carbon steel with minimum impurities. Neither contains chromium, tungsten or vanadium in the published composition.
- Carbon is the only difference: 1.25–1.35% for #1 and 1.05–1.15% for #2. Silicon (0.10–0.20%), manganese (0.20–0.30%), phosphorus (≤0.025%) and sulphur (≤0.004%) are the same.
- Heat treatment is the same on paper: annealing at 740–770 °C, quenching from 760–800 °C in water, tempering at 180–220 °C. The delivery hardness differs slightly — 223 HBW or under for #1 and 217 or under for #2 — and both reach 60 HRC or over when hardened.
- The maker grades them “highest hardness” (#1) and “high hardness” (#2). Its application lists name tipped tools, chisels and razors for both, and planes for #1; neither page lists kitchen knives, although both are widely used for them. Shirogami #3, the lowest-carbon grade, is the one Proterial lists for kitchen knives.
- More carbon leaves more carbon in solution and more cementite, which Knife Steel Nerds links to lower toughness. With no tungsten or vanadium carbides, neither grade has the wear resistance the maker attributes to the Blue steels.
- Neither grade has a published CATRA edge-retention result, and we found no test that measures #1 and #2 side by side.
Water quench and the smith
Proterial lists water — with no oil option — as the quenchant for both White steels, while it allows water or oil for the Blue steels. How hard the finished edge ends up depends on the smith’s quench and temper, not on the grade number alone.
Because the steels differ only in carbon, the choice between them is often the smith’s, made for the kind of knife he forges. If a shop publishes the finished HRC, compare that rather than the grade number.
Which should you choose?
| If… | Look at |
|---|---|
| You want the higher hardness the maker describes, and you sharpen often | Shirogami #1 |
| You want a little more toughness at a slightly lower hardness | Shirogami #2 |
| You want added wear resistance at the same carbon | Aogami #1 or #2 (Blue steel) |
| You do not want to dry the knife after every use | Neither — look at a stainless steel such as Ginsan |
The steel is only part of a knife: the knifemaker’s heat treatment, the blade geometry and the edge angle matter as much. See all steels in the Japanese knife steel chart, compare Japanese knife shapes, and if you are ordering from Japan, check the import duty calculator and buying guide first.
Frequently asked questions
- Is White #1 better than White #2?
- They differ only in carbon (1.25–1.35% vs 1.05–1.15%). Proterial calls #1 “highest hardness” and #2 “high hardness”. More carbon usually means a harder edge and lower toughness, so #1 suits careful use and #2 is a little more forgiving.
- Does Shirogami steel rust?
- Yes. Neither grade contains chromium in Proterial’s published composition. Dry the knife after every use and expect a patina.
- What does Shirogami mean?
- Shirogami means “white paper” in Japanese. In English the grades are usually called White steel #1 and #2, or White paper steel.
- What is the difference between White #2 and Blue #2?
- They share the same carbon range (1.05–1.15%). Blue #2 adds tungsten (1.00–1.50%) and chromium (0.20–0.50%) for wear resistance, according to the maker. See our Blue vs White steel comparison.
More comparisons
- Blue vs White steel
- Aogami Super vs SG2
- VG-10 vs SG2
- Blue #1 vs Blue #2
- VG-10 vs AUS-10
- Aogami Super vs Blue #2
- Ginsan vs VG-10
- HAP40 vs SG2
- SLD vs VG-10
Sources
- Proterial grade page
- Proterial grade page
- Knife Steel Nerds: is Blue Super actually super? (tungsten carbides, carbon and toughness) (secondary)
- Spark testing: how carbon, tungsten and chromium change grinding sparks (Wikipedia, with its references) (secondary)
Checked 2026-10-21. Found a better source or an error? Tell us.